Workshop, tools and materials › Lesson 9 of 18 · 12 min read

Heat treatment: annealing, hardening, tempering and case hardening

Heat treatment turns soft, easily shaped steel into hard, wear-resistant steel and back again. It is how a clockmaker makes a pivot, a pallet or a punch from a bar of silver steel. The method is simple, but the steel only does what the metallurgy says it will, so this lesson starts with what is happening.

What heat does to steel

Steel is iron with carbon dissolved in it. At room temperature the iron is in a body-centred cubic form (ferrite) with carbon locked in hard iron carbide (cementite) and the mix is relatively soft. When heated above a critical temperature (roughly 730-800 °C for silver steel; Erasteel's data sheet gives 770-790 °C as the hardening temperature), the structure changes to austenite, a face-centred cubic form that dissolves the carbon. Quenching (rapid cooling) traps the carbon before it can escape, forcing the iron into martensite, a highly strained, very hard and brittle structure. Slow cooling lets the carbon separate out, so the steel returns to a soft state.

A rough magnet test helps you recognise the critical temperature in the workshop. Plain carbon steel becomes non-magnetic as it passes through its critical range (roughly 730-770 °C), which is where the structure changes to austenite. A piece that is red hot and no longer attracts a small magnet has reached the range; take it a little past (to bright cherry red) and quench. This is a standard smith's check (typical practice, varies) rather than a precise measurement. Test with a magnet on a stick, not by hand.

The four processes

Temperatures in this lesson are approximate; the colour of the steel is the practical guide.

ProcessHeat toCoolResult
AnnealingJust above critical temperature (dull to cherry red glow)Very slowly, in the fire, in ash or vermiculiteSoft, easy to cut and drill, stress removed
HardeningBright cherry red glow, about 770-790 °C for silver steel (Erasteel data sheet; the colour is only a guide)Quench in water or oilVery hard, brittle, possibly stressed
TemperingRe-heat gently after hardening until the straw-to-blue oxide colours appear (roughly 200-320 °C, approximate)Air or water, no effect on hardnessToughness restored, some hardness lost
NormalisingAbove critical temperatureStill airEven structure, relieves stress

Overheating is more damaging than slight underheating: steel kept far above its critical temperature grows coarse grain, and beyond that it burns, with sparks and a ruined, crumbly structure.

Quench media

MediumCooling speedNotes
Brine (salt water)FastestMost severe; risk of cracking
WaterFastFor silver steel and simple shapes; can crack thin or irregular parts
Oil (mineral quenching oil)ModerateLess distortion and cracking; oil-hardening steel (gauge plate) is designed for it; hot oil can flare, so use a deep metal container with a lid
AirSlowFor air-hardening tool steels only

Quench the piece moving (stirring in a figure of eight) to break vapour jackets and cool evenly. Insert thin sections and long pieces end first and vertically, to reduce warping. Quench small parts of silver steel in oil if cracking is a risk.

Heat colours: tempering colours and glow colours

This one table covers every colour you will use, in the order steel shows them as it is heated. There are two different kinds of colour in it. When bright, polished steel is heated in air it grows a thin oxide film whose colour changes with temperature: pale straw, then brown, purple and blue. These oxide colours, from straw to blue, are the tempering colours. You polish the hardened part bright, heat it gently, watch the colours run, and cool it when the right one appears. Beyond blue the oxide colours fade to greys, and at higher temperatures the steel starts to glow. The greys and the glowing reds and oranges beyond the tempering colours are heat colours, and they mark annealing and hardening temperatures rather than tempering.

All temperatures below are approximate. I found no standard that assigns temperatures to the colours, and published tables differ by a few tens of degrees, because colour depends on steel composition, time at temperature, surface finish and, for the glow colours, the observer and the light (treat those as plus or minus 50 °C or more; work in a dim light). The temperatures and the clock uses in the right-hand column are typical practice, varies: they are indicative suggestions from workshop practice, not part of any published standard, and individual restorers differ. What is well documented is the colour sequence (light straw, straw, dark straw, brown, purple, dark blue, light blue, in order of increasing oxide thickness) and that blue can form between roughly 260 and 370 °C depending on how long the steel is heated, according to the US National Bureau of Standards.

ColourKindApprox. temperature (°C)Typical clock use
Light yellowTempering (oxide)about 210Hard tools, scribers, punches (very hard)
StrawTempering (oxide)about 220Pallet faces, pivot burnishers, cutting tools, files
Dark yellowTempering (oxide)about 240Screwdrivers for small work, punches
Yellow-brownTempering (oxide)about 250Pinion leaves, pivots
Red-brownTempering (oxide)about 260Pins, chisels, drifts
PurpleTempering (oxide)about 270Screwdrivers, hammers, general tools
VioletTempering (oxide)about 280As purple, a little tougher
Dark blueTempering (oxide)about 290Springs, tough tools, hands
Wedgwood / light blueTempering (oxide)about 300-310Springs, bluing for decoration
Grey-blue, then grey-greenBeyond tempering: the part is now softabout 320-330Very soft; mostly a decorative effect
Just visible red glowHeat colourabout 500-550Stress relieving some steels
Dull or dark red glowHeat colour (annealing)about 600-700Softening (annealing) the end of a mainspring; below hardening temperature
Cherry red glowHeat colour (annealing and hardening)about 750-800Annealing and hardening carbon steels
Bright cherry / orange-red glowHeat colour (hardening)about 850Upper hardening range, forging begins
Orange glowHeat colourabout 900-1000Case hardening, forging
Yellow glowHeat colourabout 1100Forging; too hot for small tools

Overheating is more damaging than slight underheating: steel kept far above its critical temperature grows coarse grain, and beyond that it burns, with sparks and a ruined, crumbly structure.

Furnace data are more reliable than colours: the Erasteel data sheet gives about 63-65 HRC after tempering silver steel at 150 °C and 55-57 HRC at 300 °C (see the hardening lesson for the full table). Clock-specific uses vary by maker; the right figure for a pivot is a matter of balance between wear resistance and brittleness. Many repairers temper silver-steel pivots to a dark straw or brown colour for hardness, and use blue-tempered stock where springiness matters (typical practice, varies).

Colours depend on the time and the surface. The oxide film thickens with time as well as temperature, so slow heating gives the same colour at a lower temperature. Heat gradually and quench the moment the target colour appears across the whole piece. Alloy steels, and stainless steel, colour differently. These notes apply to the oxide (tempering) colours. Surfaces must be bright and clean (no oil, no fingerprints) for the colours to appear properly.

Equipment and safe practice

Worked project 1: making a pivot burnisher (home-made pivot file)

A true pivot file has cut teeth made by specialist equipment, and is bought. What you can make well at home is a pivot burnisher with a fine, lightly grained face. It is both a polishing tool and a gentle corrective tool.

  1. Material: a piece of silver steel, say 6 mm round, 100 mm long, or a gauge-plate strip 6 × 3 mm.
  2. Shape (annealed): file one end to a flat blade about 3 mm wide and 1 mm thick, with one edge square and the other rounded. Grain one face lightly across the width with 600-grit paper on a flat plate, so the surface is fine and even.
  3. Handle: drive the tang into a wooden or brass handle.
  4. Harden: heat the working end to cherry red (about 770-790 °C for silver steel, Erasteel data sheet), checking the magnet test, then quench in oil, with the tip entering first.
  5. Clean: polish the face lightly with fine abrasive until it is bright again.
  6. Temper: heat gently from the thick part, not the tip, until the face turns straw (a tempering colour, about 220-230 °C), then cool.
  7. Finish: stone the edges to a smooth, square edge and a smooth rounded edge, polishing them with a fine stone and rouge. The finished edges should have no burrs.

Check: the tool should scratch ordinary mild steel with difficulty, should not chip on bumping against a brass plate, and the edge should leave no scratch lines on a test pivot of mild steel.

Worked project 2: making a replacement pallet

A pallet is the hard steel face on which an escape wheel tooth slides, so it must be hard and smooth. For a recoil or deadbeat anchor with separate, inserted steel pallets, a replacement can be made as follows.

  1. Copy the original: make a scale drawing or trace from the existing pallet; measure thickness and the angles of the faces. If the original is missing, use the matching pallet as a guide and mark the geometry from the escape wheel.
  2. Material: a piece of gauge plate (oil-hardening) of slightly greater thickness than the original, or silver steel rod filed flat.
  3. Shape: saw and file the blank to shape with the faces slightly oversize, leaving about 0.1-0.2 mm for finishing. File the faces at the correct angles using the pattern as a gauge.
  4. Harden: heat to bright cherry red and quench in oil. Handle with tongs and keep the face uniform.
  5. Clean and temper: polish a small area bright. Reheat gently to light straw (a tempering colour, about 220 °C) so the face is very hard but not glassy. Pallets typically work in the low tempering range for wear resistance, but over-hard pallets chip.
  6. Stone and polish: use a fine India or Arkansas stone, then a zinc or boxwood lap with diamantine or rouge, keeping faces flat and the angles consistent.
  7. Fit: secure the pallet in the anchor with a slot and a tiny drop of shellac, or with a pin and fine solder, without overheating.
  8. Test: check that the face is smooth under 10× magnification, that the drop onto the tooth is right, and that the clock runs and keeps its drop.

Worked project 3: making a depthing tool, with case hardening

A depthing tool measures the centre distance at which two wheels or a wheel and pinion mesh correctly, so that new pivot holes can be marked in the right place. A simple version is made from two hinged arms with adjustable centres.

  1. Parts: two flat arms of mild steel or brass (say 120 × 12 × 3 mm), a hinge pin, a thumbscrew and a knurled nut, and two sets of hardened conical centres (60° points) or fine pivot sockets.
  2. Arms: drill and ream the hinge hole (reamed to the pin), and fit the pin so the arms swing freely without side play. Drill small holes near the free ends of each arm to take a hardened centre, or file V-notches.
  3. Centres: turn short pointed centres from silver steel. Harden them (cherry red, quench in oil), temper to purple (a tempering colour), and polish the points. They must be sharp and accurate; the points are what contact the work.
  4. Case-harden the hinge pin (optional) if the pin is made from mild steel: heat to a bright orange glow (about 900 °C, approximate), roll in a case-hardening compound (for example a commercial carbon-based compound), reheat to the same temperature, hold for a few minutes, and quench in water. The surface skin, a few tenths of a millimetre deep, becomes hard while the core stays tough. Many older compounds contain cyanide salts and give off toxic fumes; use only in a well-ventilated place and follow the label.
  5. Fit a locking screw so the arms can be locked at a chosen spacing.
  6. Use: set the centres into the pivot holes of the wheel and pinion with correct end shake, adjust until the teeth mesh smoothly, lock the arms and transfer the distance with dividers to the plate for the new hole.

Case hardening in brief

Case hardening adds carbon to the surface of low-carbon steel, so that a thin outer layer can be hardened by quenching while the core remains soft and tough. For clock work it suits mild-steel parts that need a hard bearing surface: pins, studs, small pivots in non-critical places. The steps are: clean the part, heat to a bright orange glow (about 900 °C, approximate), pack or roll it in carbon-bearing compound, hold at temperature (longer gives a deeper case), then quench in water. The case depth is typically a few tenths of a millimetre for a few minutes at temperature (typical practice, varies; not from a published standard). Thin parts may warp, and sharp corners can crack.

Annealing a hard part

To drill or file a part that has hardened (for example, a hardened silver-steel pin you need to modify), heat it to a dull cherry red glow (a heat colour, not a tempering colour) and cool as slowly as possible, by burying it in dry vermiculite, lime or ashes, or by shutting off the furnace and leaving it to cool. Do not quench. After machining, harden and temper again.

Common mistakes

Sources

Colour-to-temperature pairings, heat colours and case-hardening details are typical workshop practice; see the hardening and tempering lesson for furnace data from steelmakers' sheets.

Get new lessons by email