Workshop, tools and materials › Lesson 8 of 18 · 9 min read
Metals for clocks: brass, bronze, steel, iron and how to tell them apart
Nearly every clock is brass and steel, with a few other metals in supporting roles. Knowing which alloy you are holding tells you how it will file, turn, bend, harden and corrode, and which replacement stock to buy. This lesson covers what the metals are, why they behave as they do, and how to identify an unknown piece.
Why alloys matter: a short primer
A pure metal is soft because planes of atoms slide over one another easily. Adding a second element distorts the crystal lattice and resists that sliding, so alloys are usually stronger and harder than the pure metals. Work hardening (cold working) does the same thing mechanically: hammering, rolling or drawing multiplies defects (dislocations) in the crystal so further deformation is harder. Annealing heats the metal enough to let the crystal structure recover and removes that hardening and the internal stress. Steel adds a further mechanism, heat treatment, covered in the next lesson.
Brass
Brass is an alloy of copper and zinc. The composition controls colour and properties. The Copper Development Association notes that alloys with at least about 63% copper (up to about 35% zinc) form a single alpha phase that is ductile and can be cold worked, while alloys with around 35-45% zinc contain both alpha and beta phases, which are less ductile cold but easier to work hot. More zinc gives a yellower, cheaper and stronger metal that is more prone to dezincification (the zinc leaching out and leaving porous copper).
| Brass | Approximate composition | Properties and clock uses |
|---|---|---|
| Gilding metal | 80-95% copper, remainder zinc | Gold-like colour; soft, easily worked; used for some decorative parts and as a gilding base |
| Cartridge brass (70/30) | About 70% Cu, 30% Zn | Very ductile; sheet for forming, hands and cases; susceptible to season cracking |
| Common brass (63/37; CZ108 in the old British designation) | About 63% Cu, 37% Zn | Cold-working brass for sheet, strip and wire |
| Muntz (60/40) | About 60% Cu, 40% Zn | Stronger, hot-workable, bright yellow; found in rod and plate, not ideal for cold-forming |
| Free-cutting (leaded) brass (CZ121 Pb3) | About 58% Cu, 39% Zn, 2.5-3.5% Pb | Machines to a fine finish with short chips; used for engraving brass, bushes, screws and pillars; not suited to hammering or bending |
| Clock plate brass (historic) | Varies; often a copper-zinc brass cast and hammered, later rolled | Hammer-hardened plates are stiff; hammering leaves residual stresses |
Cast and hammered brass, used in many 17th and 18th century clocks, carries internal stress from hammering. Rolled sheet of the 19th century has more even stress but is not stress-free. The Copper Development Association states that lead improves machinability (the lead breaks chips into small pieces and acts as an internal lubricant) and lowers friction and wear; that is why leaded brass is common in instrument and clock work (typical practice). A small amount of lead is generally acceptable for gears and plates, though lead is a safety concern in filing and soldering dust (see the safety lesson).
Season cracking
Season cracking is stress-corrosion cracking of brass. The term is traditionally said to come from the failure of brass cartridge cases of British forces in India in the monsoon season (a widely repeated account that We could not verify in the primary sources). A major study of the problem was published in 1921 (Moore, Beckinsale and Mallinson, Journal of the Institute of Metals), and US Bureau of Standards work of 1924 connected the cracking with internal stress left by cold working. A US Office of Naval Research review notes that ammonia is one of the conditions needed for ammoniacal stress-corrosion cracking, alongside water, oxygen, tensile stress and a susceptible alloy, and that brass with more than about 20% zinc is rated highly susceptible.
Two conditions are needed: residual tensile stress and a corrosive agent. A clock plate that has been hammered and has never been stress-relieved is stressed; ammoniated cleaning fluid, or ammonia vapour from cleaning products and old polishes, supplies the second. The cracks can appear hours or days after cleaning, and you may find a crack in a plate that was sound when it went in. Annealing after forming relieves the stress: Bureau of Standards work on brass tube found that a low-temperature anneal of a few hours at about 300-325 °C released most internal stress without much loss of hardness, whereas a full anneal at 400 °C softened the metal. You cannot do either to an antique plate without risking its surface and character. For valuable old plates, avoid ammonia, use a dilute, ammonia-free cleaner, and rinse thoroughly.
Working brass
- Work hardening: brass hardens when bent, hammered or rolled. A hardened spring part (such as a rack tail or a friction spring) is deliberately left hard; a part that must be formed should be annealed first.
- Annealing: heat to a dull red, at about 450-600 °C (typical practice, varies with the alloy), in a dim light so the glow is visible, then let it cool or quench; quenching brass does not harden it.
- Fingerprints: acids and salts in skin etch brass, leaving prints that are hard to remove. Handle clean brass with a cloth or gloves.
Bronze and other copper alloys
| Alloy | Composition | Clock use |
|---|---|---|
| Tin bronze (including bell metal) | Copper with 10-20% tin | Bells, gongs, gears in some turret clocks, bearings |
| Phosphor bronze | Copper, tin, a little phosphorus | Bushes, springs, wear parts; hard and elastic |
| Gunmetal | Copper, tin, zinc | Castings, large bearings and wheels |
| Nickel silver ("German silver") | Copper, nickel, zinc (no silver) | Dial and decorative parts |
| Beryllium copper | Copper with about 2% beryllium | Springs; hazardous dust when machined |
Steels
Steel is iron with carbon (up to about 2%) and possibly other alloying elements. Carbon content governs how hard the steel can be made by heat treatment: below about 0.3% carbon it hardens little, and above about 0.7% it can reach very high hardness at the cost of toughness.
| Steel | Carbon / alloy | Condition | Clock uses |
|---|---|---|---|
| Mild steel (low carbon; for example EN1A or similar free-cutting grades) | About 0.1-0.25% C | Does not harden by quenching; can be case-hardened | Pillars, studs, screws for non-wearing parts, arbors that are not pivots, bench blocks |
| Silver steel (BS 1407) | About 0.95-1.20% C with chromium and manganese (Erasteel) | Supplied soft, ground bright round bar; hardens to about 64-66 HRC (Erasteel gives 66) | Pivot steel, pins, punches, small tools, pallets, pinion arbors, staffs |
| Gauge plate (oil-hardening flat ground stock) | About 0.9-1.0% C with manganese, chromium, tungsten | Flat ground to thickness; oil-hardening, little distortion | Pallets, anchors, gauges, small cutters |
| Blue (tempered) steel | High carbon, ready hardened and tempered to blue | Springy and tough; not hardened further | Hands, pivots and staffs for light duty, springs, pins |
| Spring steel (high-carbon or alloy) | About 0.6-1.0% C | Hardened and tempered for elasticity | Mainsprings, click springs, hairsprings (older) |
| Stainless steel (austenitic, 304-type) | Chromium, nickel; low carbon | Non-magnetic or weakly magnetic; does not harden by quenching | Modern mainsprings, screws, replacement pins; tools |
| Modern watch spring alloys | Cobalt-nickel-chromium and similar | Hardened by cold work and ageing; non-magnetic, rust-resistant | Modern hairsprings and mainsprings |
| Cast iron | 2-4% C, with flakes of graphite | Brittle; machined with sharp tools; cannot be forged or bent | Turret clock frames, large wheels, bases, weights |
| Wrought iron | Very low carbon, with slag fibres | Soft, fibrous, forgeable | Early clock frames, bars, large gear arbors |
The silver steel composition is a published standard (BS 1407, published by BSI in 1970). Silver steel contains no silver; the name refers to its polished, bright appearance. The Erasteel data sheet for silver steel gives about 66 HRC as the maximum hardness after hardening and an approximate as-supplied Brinell hardness of 180-285; manufacturers' data sheets will give details for the batch you buy.
Magnetism
Iron and most steels are magnetic, and parts can become magnetised, which in a watch balance spring ruins timekeeping because coils cling together. Clocks with large pendulums are less sensitive, but a magnetised steel part will attract steel swarf and can interfere with escapement parts. Demagnetise with a demagnetising coil. Austenitic stainless steel is generally non-magnetic or only weakly magnetic, though cold working can make it slightly magnetic.
How to identify an unknown metal
- Colour: pink-red is copper; yellow is brass (paler yellow means more zinc); reddish-brown is bronze; white-silver is nickel silver or stainless.
- Magnet test: sticks to the magnet means iron or steel (not brass, bronze or aluminium). Stainless varies.
- File test: a file bites into soft, annealed steel and brass; it skates over hardened steel.
- Spark test: a grinding wheel throws bright, branching sparks from high-carbon steel, orange straight sparks from mild steel, and none from brass.
- Weight: brass is about 8.4-8.7 g/cm³, steel about 7.85 g/cm³, aluminium about 2.7 g/cm³. Weigh a piece and measure its volume.
- Sound: brass gives a dull note, bronze and steel a ringing one.
- Machining behaviour: leaded brass gives small broken chips; ordinary brass gives long curls.
- Hardness test: try a file, a scribe or a centre punch.
Common mistakes
- Choosing free-cutting brass for a part that must bend or be riveted; it cracks.
- Using mild steel where silver steel is required and hoping to harden it.
- Cleaning hammered brass plates in strong ammonia solutions.
Sources
- Introduction to Brasses, Part I (Copper Development Association)
- Introduction to Brasses, Part II (Copper Development Association), for lead as the reason free-cutting brass machines to short chips
- R. J. Anderson and E. G. Fahlman, Release of internal stress in brass tubing, Technologic Paper T-285 (US Bureau of Standards, 1924)
- B. F. Brown, Stress corrosion cracking control plans, 3. Copper alloys (Office of Naval Research / NTIS, 1975)
- Moore, Beckinsale and Mallinson, The season-cracking of brass and other copper alloys, J. Inst. Metals 25, 35-152 (1921) (bibliographic record, Smithsonian Museum Conservation Institute)
- Erasteel STUBS Silver Steel data sheet (Erasteel; copy hosted by a distributor)
- BS 1407:1970 Specification for high carbon bright steel (silver steel) (BSI)
The table of brass, bronze and steel grades and typical uses is summarised from general materials practice; compositions of named grades vary by standard and supplier.
Get new lessons by email
Free, practical clock repair lessons for beginners. No spam, unsubscribe any time.